Molybdenum TZM Alloy Properties and Applications

Molybdenum TZM mechanical physical properties specifications chemistry

EFINEA Metals supplies molybdenum TZM to OEMs and engineering teams in aerospace, heat treating, die casting, and medical imaging. This page puts the technical data and applications for TZM alloy in one place so engineers can evaluate the material and purchasing teams can confirm form and specification.

For property data beyond this page or help matching a size range to a drawing, call our sales engineers and metallurgists at 1-800-348-6268. As a TZM distributor serving high-technology industries since 1965, EFINEA stocks the alloy in plate, sheet, round bar, and rod.

Molybdenum TZM Properties

TZM is named for titanium, zirconium, and molybdenum, with a small amount of carbon added. These additions form fine carbide particles that pin the grain structure, giving TZM roughly twice the high-temperature strength of unalloyed molybdenum and raising its recrystallization temperature by about 300°C.

Engineers usually switch to TZM material when pure molybdenum would recrystallize or creep under the heat and load of the application.

The tables below cover physical properties, mechanical properties for plate, sheet, bar, and rod, chemistry, and the governing specifications. Download the EFINEA Molybdenum TZM data sheet from the Data Sheets section of our Technical Library.

Typical Physical Properties

Physical properties describe how TZM behaves as a bulk material with no load applied. Because the alloying additions total less than 1%, most of these values sit close to those of pure molybdenum. 

Density and melting point are nearly identical. The recrystallization temperature is where the two materials differ most, and it is the reason TZM exists.

Molybdenum TZM Typical Physical Properties

Densitylb/in30.37

g/cm310.22
Melting Point°F4753
°C2623
Electrical ResistivityMicrohm-cm6.85
Thermal Conductivity @20°CCal/cm2/cm°C/sec0.48
Specific HeatCal/gm/°C0.073
Recrystallization Temp°C1400
Coefficient of Linear Thermal ExpansionMicro-in/°F x 10-6 2.50
Micro-in/°C x 10-65.20
Source: MatWeb, Plansee

Recrystallization is the point at which heat causes a new, coarser grain structure to form, and strength and room-temperature ductility drop as a result. Pure molybdenum recrystallizes at about 1100°C. 

TZM maintains its worked structure up to about 1400°C, extending the range over which the material retains its full strength. The low coefficient of thermal expansion, roughly one-third that of stainless steel, keeps TZM components dimensionally stable through repeated heating and cooling, and the high thermal conductivity pulls heat away from hot surfaces. Both properties matter in die casting and furnace work, where parts cycle through large temperature swings.

Typical Mechanical Properties, Plate and Sheet

The values below are ASTM B386 minimums for TZM plate and sheet in the stress-relieved condition, tested at room temperature. Stress-relieved material keeps the strength gained from rolling, which is why it is the standard supply condition for structural and tooling applications. Requirements vary by thickness, so purchase orders should reference the thickness range alongside the specification.

Molybdenum TZM Typical Mechanical Properties - Plate + Sheet

FormSheet Thickness
in. (mm)
Tensile Strength
min, ksi (MPa)
Yield Strength
0.2 % Offset, min.
ksi (MPa)
Elongation
2" (50 mm), min. %
Plate
0.187" to 0.500"
(4.750 to 12.700)
120
(830)
100
(690)
10
0.500" to 1.000"
(12.700 to 25.400)
110
(760)
95
(660)
10
Sheet
0.025" to 0.060"
(0.635 to 1.524)
120
(830)
100
(690)
7
0.060" to 0.090"
(1.524 to 2.286)
120
(830)
100
(690)
9
0.090" to 0.187"
(2.286 to 4.750)
120
(830)
100
(690)
10
Source: ASTM B386 Type 364 (Plate, Sheet), Table 3 Stress Relief; When tested between 65° and 85 °F (18° and 29 °C)

Thinner sheet shows lower minimum elongation, because thin gauges exhibit more directional grain structure from rolling. Thicker plate has a slightly lower strength minimum, since heavier sections undergo less reduction during processing.

Mechanical Properties, Bar and Rod

ASTM B387 sets minimum properties for TZM bar and rod by diameter. Strength and elongation both step down as diameter increases, for the same reason as with plate: larger sections receive less working. 

This table also includes a hardness range, which is useful for receiving inspection and for estimating tool wear before machining.

Molybdenum TZM Mechanical Properties - Bar + Rod

Diameter, in. (mm)Tensile Strength,
min. ksi (MPa)
Yield Strength,
0.2 % Offset, min.
ksi (MPa)
Elongation in 1"
(50 mm) %
Hardness (DPH),
-10 kg, Vickers-10 kg
0.188" to 0.875"
(4.76 to 22.2)
115
(790)
100
(690)
18260 - 320
0.875" to 1.125"
(22.2 to 28.6)
110
(760)
95
(655)
15250 - 310
1.125" to 1.875"
(28.6 to 47.6)
100
(690)
85
(585)
10245 - 300
Source: ASTM B387 Type 364 (Bar, Rod), Table 3 Stress Relief

Compared with unalloyed molybdenum, TZM shows a higher room-temperature yield strength, and the gap widens as temperature rises. That retained strength at furnace and tooling temperatures is what most buyers are paying for when they specify TZM over pure molybdenum.

Chemistry

TZM’s performance depends on keeping its additions inside narrow limits. Titanium and zirconium react with carbon to form the carbide particles that strengthen the alloy and resist recrystallization. Too little carbon, and the carbides do not form in sufficient quantity. Too much and the material loses ductility.

Molybdenum TZM Chemistry

Molybdenum (Mo)Balance
Titanium (Ti)0.40 - 0.55
Zirconium (Zr)0.06 - 0.12
Carbon (C)0.01 - 0.04
Source: ASTM B386 ASTM B387 Type 364, Table 1

Every TZM shipment from EFINEA includes mill certifications, and chemistry can be verified with handheld XRF equipment at our warehouses when traceability is a program requirement.

Specifications

TZM is designated Type 364 in both ASTM molybdenum product specifications. ASTM B386 covers plate and sheet, and ASTM B387 covers round bar and rod. The UNS number is R03640.

Molybdenum TZM Specifications

ASTM B386 Type 364
(Sheet + Plate)
ASTM B387 Type 364
(Round Bar)
UNS R03640

For full background, the websites of ASTM International and ASM International publish the technical standards governing TZM. If a drawing calls out a superseded or unfamiliar designation, contact our sales team for help with the cross-reference.

Molybdenum TZM Applications

TZM alloy is specified for work that combines high temperature with mechanical load, typically from 1000°C to 1400°C in vacuum or a protective atmosphere.

In that range, TZM’s higher strength and creep resistance keep components in shape where pure molybdenum would sag or deform. The sections below cover the most common uses and the property that drives TZM’s selection in each.

Structural Furnace Components

Vacuum and hydrogen-atmosphere furnaces use TZM for load-bearing hot-zone hardware: support rails, hearth plates, fixtures, racks, trays, and fasteners. These parts carry the workload through long, high-temperature cycles, and creep resistance determines how long they stay flat. 

Furnace builders often pair pure molybdenum heat shields with TZM structural members, using the stronger alloy only where load requires it. TZM threaded rod and nuts are common in hot zones because they share the thermal behavior of the surrounding molybdenum structure.

Rotating Anodes for X-Ray Tubes

Rotating anodes in medical CT and diagnostic X-ray tubes are commonly built on a TZM base with a tungsten-rhenium focal track. The electron beam strikes the focal track, generating intense localized heat, and the TZM body carries and spreads that heat while spinning at high speed. 

TZM’s strength at temperature keeps the anode from distorting under centrifugal load, and its lower density compared with tungsten reduces the rotating mass the bearings must support.

Rocket Nozzles and Aerospace Components

Rocket nozzles, nozzle throat inserts, heat shields, and leading edges use TZM where structural parts must hold strength during short, intense exposure to hot combustion gases. TZM offers a strength-to-weight advantage over tungsten for parts that do not reach tungsten’s temperature range.

Extrusion Dies and Hot Runner Components

Extrusion dies for brass and copper alloys use TZM for its high strength at elevated temperatures and resistance to wear from the billet. In plastics injection molding, TZM hot runner nozzle tips use the alloy’s thermal conductivity to keep resin temperature uniform.

Die Inserts for Aluminum Die Casting

TZM die inserts and cores are used in aluminum die casting, where steel tooling wears quickly. Heat checking, the network of fine cracks that forms from repeated thermal shock, is a main cause. 

TZM’s high thermal conductivity pulls heat out of the casting faster, and its low thermal expansion limits the stress each cycle puts on the insert surface. That means longer insert life and less downtime in high-volume casting cells. TZM also resists soldering, where molten aluminum bonds to the die surface.

Hot Stamping and Forging Tooling

Isothermal forging and hot stamping of titanium alloys and nickel-based superalloys use TZM dies, often in vacuum or an inert atmosphere. In isothermal forging, the die and workpiece are held at the same high temperature, so the metal forms slowly without cooling against the tooling. 

Few tool materials keep enough strength at those temperatures. TZM does, which makes it a common choice for forging aerospace turbine disks and structural components.

Electrodes

TZM electrodes are used in high-temperature processes where the electrode must carry current while resisting deformation. Its heat resistance allows electrodes to maintain their geometry longer than unalloyed molybdenum under demanding duty cycles.

Why Source TZM from EFINEA Metals

EFINEA Metals has supplied refractory metals to high-technology industries since 1965. As a molybdenum TZM supplier with inventory across four ISO 9001:2015 and AS9100D certified facilities in New Jersey and California, we ship standard stock within 24 hours of order confirmation. 

Buyers comparing TZM suppliers often weigh traceability as heavily as price, and every EFINEA shipment includes mill certifications to ASTM B386 or B387. Our in-house cutting produces near-net-size blanks that cut machining time on a material that is hard on tooling, and our metallurgists can advise on grade selection and specification interpretation.

Frequently Asked Questions About Molybdenum TZM

Specify TZM when a part carries load at temperatures above roughly 1000°C, or when service temperatures would recrystallize pure molybdenum and leave it weak and brittle at room temperature. For heat shields and other parts that experience high temperatures without significant load, pure molybdenum is usually adequate and less expensive.

Both raise the recrystallization temperature of molybdenum, but by different mechanisms. TZM relies on titanium and zirconium carbides and offers higher strength at moderate high temperatures. Molybdenum-lanthanum oxide (MoLa) uses a dispersion of lanthanum oxide particles and tends to retain better ductility after recrystallization, which makes it a common choice for sheet components that are formed or that see temperatures above TZM’s range.

TZM can be fusion-welded by electron beam or gas tungsten arc processes in a protective atmosphere, but the weld and heat-affected zone recrystallize and lose ductility. For structural assemblies, mechanical fastening or brazing is usually preferred. If welding is required, design the joint away from high-stress areas.

Yes. TZM’s higher strength and hardness increase tool wear, so carbide tooling and rigid setups are standard. Grinding and EDM are common for close tolerances. Buying near-net-size blanks reduces the amount of material that must be removed.

Yes. Like pure molybdenum, TZM oxidizes rapidly in air above roughly 500°C, forming a volatile oxide. High-temperature service should take place in vacuum or a protective atmosphere such as hydrogen or argon. Parts that must operate in oxidizing conditions require a protective coating.

TZC is a related molybdenum alloy with higher titanium, zirconium, and carbon content. It offers greater strength at very high temperatures but is harder to fabricate and less widely available. TZM is the more common choice and is covered by ASTM B386 and B387 Type 364.

At minimum, list the form, dimensions and tolerances, the governing specification (ASTM B386 Type 364 for plate and sheet or ASTM B387 Type 364 for bar and rod), and the condition, which is typically stress relieved. Note any certification or surface finish requirements. Our sales team can review a drawing or an RFQ before ordering.

Standard stock items ship within 24 hours of order confirmation. Lead time for custom-cut material depends on the complexity of the order and the current shop workload. Your sales contact can confirm lead time at the time of your quote.